Silicon, Sandelin and Sebisty: Reading the Mill Certificate Before It Costs You
Two numbers on the mill certificate, silicon and phosphorus, decide most of what a galvanized coating will look like and how much zinc it will take. How ISO 14713-2 and ASTM A385 read them, why the silicon equivalent matters, what reactive steel costs in kilograms per tonne, and what to write into the order.
The certificate is the first inspection
Most of what a galvanized coating will look like is decided at the mill, by two numbers on the certificate: silicon and phosphorus. The kettle, the pickling line and the immersion time can be identical, and one heat still comes out bright at about 65 µm while the next comes out dull grey at 200 µm or more.
This article reads the certificate the way a galvanizer has to, before the steel is on the gantry. What it settles:
- ISO 14713-2 sorts steel into four categories by silicon and phosphorus, and ASTM A385 recommends silicon targets of its own. The two draw their lines in different places.
- Phosphorus counts 2.5 times as much as silicon. ISO 14713-2 Table 1 NOTE 1 uses the silicon equivalent, Si + 2.5P, to decide whether low-silicon steel still behaves as category A. It is the number to calculate.
- A certificate is one sample from a heat. Near the steep part of the curve, a difference of 0.02% silicon changes the coating, and ASTM A385 itself says the certificate is an indication, not a guarantee.
- Reactive steel costs zinc before it costs appearance. On 8 mm work, every 50 µm over the design coating is 11.4 kg of zinc per tonne.
- Nickel in the bath is a costed proposal for the whole plant, not a fix for one heat. Reactive steel should be priced on its own line.
- In the order, ask for the numbers. Do not write them in as an acceptance limit.
Four ranges, four behaviours
ISO 14713-2:2020 Table 1 sorts steel into four categories for galvanizing at 440 to 460 °C. The letters do not run in order of silicon, so the table below is sorted by silicon instead.
| ISO category | Silicon and phosphorus, % | What the coating does | Typical thickness, µm |
|---|---|---|---|
| A | Si ≤ 0.03 and P < 0.02 | Shiny, finer texture, outer zinc layer present | 38 to 64 |
| C | Si above 0.03 to below 0.14 | Excessively thick, darker and coarser. Iron-zinc alloy dominates and often reaches the surface, with reduced resistance to handling damage. The Sandelin region of ASTM A385 lies inside this category | 100 to 200 or more, erratic |
| B | Si 0.14 to 0.25; P above 0.035 raises reactivity | Shiny or matt, the outer zinc layer may or may not survive. ASTM A385's upper target window of about 0.15 to 0.22% lies inside it, where the Sebisty effect keeps coatings moderate | 64 to 100 |
| D | Si above 0.25 | Thickness rises with silicon | 100 to 250 or more |
The thickness column is the typical range from V&S Galvanizing's chemistry guide, which cuts its bands at 0.04, 0.15 and 0.22% silicon. Treat it as an order of magnitude, since section thickness and immersion time move it.
Table 1 NOTE 1 widens category A in one direction. Steel with silicon at or below 0.03% whose silicon equivalent, Si + 2.5P, is at or below 0.09% is also expected to behave as category A. For cold-rolled steel, the note expects that behaviour only when Si + 2.5P is at or below 0.04%. This is the reading the site's Steel Reactivity Checker applies.
ASTM A385/A385M-20 section 3.2 draws its lines differently. It names silicon between 0.06 and 0.13% as the Sandelin region and silicon above 0.25% as a second, high-silicon region, both able to produce thick, dull coatings. When steel is produced or bought for galvanizing, it calls it good practice to aim for silicon below 0.04% with a maximum of 0.06%, or for silicon between 0.15 and 0.22% with a minimum of 0.13% and a maximum of 0.25%. It adds that carbon above about 0.25%, phosphorus above 0.04% or manganese above about 1.3% will change the coating. ISO's category A stops at 0.03% and ASTM's low target at 0.04%. ISO's category B and ASTM's upper window both end at 0.25%.
Both agree on the shape: a window of well-behaved steel at low silicon, a bad region above it, a second window around 0.15 to 0.22%, and a steady climb beyond.
Two notes in ISO 14713-2 Table 1 matter for the bath. A nickel or aluminium addition to the melt can change the table's characteristics significantly, and the table says nothing useful for high-temperature galvanizing at 530 to 560 °C. Steel below 0.01% silicon with aluminium above 0.035% can react less than expected, giving thinner coatings with reduced cohesion.
Sandelin, Sebisty and the phosphorus multiplier
Silicon acts through a curve that is neither linear nor monotonic, and phosphorus acts as silicon multiplied by 2.5. Coating thickness rises steeply from about 0.04% silicon, peaks through the Sandelin region, falls back through the Sebisty window of about 0.15 to 0.22%, and climbs again above about 0.22 to 0.25%.
The steep part is the danger. The AGA points to the slope around 0.05% silicon as very steep, so the gap between 0.04% and 0.06% can be the gap between a bright coating on specification and a dull, thick one. ASTM A385/A385M-20 section 3.2 names 0.06 to 0.13% as the Sandelin region, and the Zinc Consumption KPIs article uses the same range for the steel where zeta growth is thick and uncontrolled.
The silicon equivalent folds phosphorus in:
Si equivalent = Si (%) + 2.5 × P (%)
Read it against ISO 14713-2 Table 1 NOTE 1 first: with silicon at or below 0.03% and the silicon equivalent at or below 0.09%, or 0.04% for cold-rolled steel, the steel is expected to behave as category A. ASTM A385/A385M-20 section 3.2 makes the same point in words: even when silicon and phosphorus are each held to desirable limits, the two together can give a mottled or dull grey coating.
The AGA reads the silicon equivalent more cautiously, against the same windows it uses for silicon. Below 0.04% or between 0.15 and 0.22% it expects a coating of typical thickness and appearance. Between 0.04 and 0.15% it expects a Sandelin steel, with variable appearance and thicker coatings. Above 0.22% it expects a matt grey, rough coating, thicker than the minimum. Use these windows as a flag for a test dip, not as a category. On the phosphorus side, ISO 14713-2 notes that phosphorus above 0.035% makes category B steel more reactive.
Time in the kettle works differently on the two kinds of steel. On a non-reactive steel, coating growth levels out after a few minutes. On a reactive steel, the AGA reports that growth continues for as long as the steel stays in the kettle, so a thick section that needs a long immersion to come up to temperature is where a Sandelin heat does the most damage.
Reading a certificate
The same certificate can get two readings, depending on whether you read it against ISO 14713-2 or against the AGA's silicon-equivalent windows. These six heats are illustrative, invented for this article, not taken from real certificates.
| Heat | Si, % | P, % | Si + 2.5P, % | ISO 14713-2:2020 Table 1 | AGA silicon-equivalent window |
|---|---|---|---|---|---|
| 1 | 0.020 | 0.015 | 0.058 | A; within NOTE 1 unless cold-rolled | Inside 0.04 to 0.15: flag for a test dip |
| 2 | 0.080 | 0.012 | 0.110 | C | Sandelin |
| 3 | 0.180 | 0.015 | 0.218 | B | Typical, just inside 0.22 |
| 4 | 0.180 | 0.030 | 0.255 | B, P below 0.035 | Above 0.22, thick and matt |
| 5 | 0.300 | 0.020 | 0.350 | D | High, thick and rough |
| 6 | 0.008 (Al 0.040) | 0.012 | 0.038 | Al above 0.035: thin coating risk | Below 0.04, thin coating risk |
Heats 1 and 4 are the interesting ones. ISO 14713-2 reads heat 1 as category A, on its silicon and phosphorus and again on NOTE 1, and that is the reading to plan on. The AGA's more cautious window puts its silicon equivalent of 0.058% in the Sandelin band, which is a reason to galvanize a test piece if appearance matters, not a reason to reclassify the steel. Heat 4 is category B by ISO, yet its silicon equivalent of 0.255% is above 0.22%. When the two readings disagree, the heat sits near a boundary on a steep curve. Treat the disagreement as information, and do not quietly pick the kinder reading.
The certificate also has limits that no calculation removes:
- One sample. The AGA and V&S both note that a mill test report is a single sample from a heat, and that element levels vary by about ±0.02% through a heat and even across one piece. A reported 0.04% silicon can mean 0.02% or 0.06% on the piece in front of you.
- An indication, not a guarantee. ASTM A385/A385M-20 section 3.2 says the silicon values in mill test reports can indicate the steel's reactivity but are not a guarantee, and that the best practice is to galvanize test pieces. The AGA and V&S both warn that some certificates, from certain foreign producers in particular, do not reflect the steel delivered.
- Mixed steels. A fabrication can combine several heats and grades, and each element of it reacts on its own chemistry. ASTM A385/A385M-20 section 4.1 asks that assemblies consist of steels of similar chemistry and surface condition wherever possible.
Three rules follow. Calculate the silicon equivalent for every heat, not silicon alone. Treat any value within 0.02% of a boundary as uncertain. When the chemistry is in doubt, galvanize a representative test piece before committing the lot, which is the advice of ASTM A385, the AGA and V&S alike.
What reactive steel does to the coating
Reactive steel gives a thicker, duller, less forgiving coating, and every micron above the design thickness is zinc the plant pays for. The structure explains the look. ASTM A385/A385M-20 section 3.3 describes it as accelerated growth of the compound layers, the zeta layer in particular, with the outer zinc layer virtually gone, which is seen as a grey matte finish instead of the usual bright one. A large surface can show matte and bright areas side by side, a mottled appearance.
The same structure explains the handling problem. ISO 14713-2 describes category C coatings as iron-zinc alloy reaching the surface, with reduced resistance to handling damage, and ASTM A385/A385M-20 section 3.4 notes some evidence that these coatings are more brittle and less adherent than normal ones. The AGA puts the practical limit at about 250 µm, above which thick members such as beams and poles can flake under handling, assembly or shipping. Weathering steels such as A588 and A709 50W are reactive by design: the AGA gives up to 0.40% silicon allowed and 0.27 to 0.35% as common, with a matt grey coating, and V&S reports coatings of 100 to 200 µm or more.
Dull appearance and minor roughness that follow from the steel are not grounds for rejection. ASTM A123 section 6.2 says that roughness related to steel chemistry or reactivity shall not be grounds for rejection, and ISO 1461:2022 clause 6.1 says that darker or lighter areas and some unevenness are not a cause for rejection. Neither excuses everything: ISO 1461 still rejects roughness or sharp points that can cause injury. That protects the galvanizer within limits, and it is one more reason to put thickness, not looks, at the centre of the order.
The zinc is where it hurts. Using the formula from the Zinc Consumption KPIs article, with surface area of about 255 divided by the section thickness in mm, 8 mm work carries about 31.9 m²/t. The extra zinc per tonne for a given excess thickness is then:
| Excess over design coating, µm | Extra zinc, kg/t (8 mm work) | Zinc consumption points |
|---|---|---|
| 25 | 5.7 | 0.57 |
| 50 | 11.4 | 1.14 |
| 100 | 22.8 | 2.28 |
The plant-wide effect depends on the share of reactive tonnage. If 10% of a 500 t month is Sandelin steel running 50 µm over the design coating, the extra zinc is about 570 kg a month, or 0.11 points on the blended consumption figure. That sounds small. It is concentrated on a few customers' steel, and that is the point of the pricing section below.
The KPI article also makes the cost point in one line: for Sandelin steel the dominant cost is coating thickness on the product, not bath dross.
Nickel in the bath is a costed proposal
Nickel suppresses the Sandelin effect, but it is a bath-wide decision whose costs land on every tonne, not a repair for one heat. The AGA notes that nickel is most commonly added to control reactive steel by reducing intermetallic growth, and that it works while the steel's silicon is below about 0.20%. V&S puts the working level at 0.04 to 0.06% nickel, and the KPI article uses about 0.05%.
The costs are specific.
- Dross. The AGA gives 0.05% as a critical maximum for a kettle running at 440 °C, to avoid excessive dross formation. The dross buyer needs briefing first, because nickel changes dross chemistry.
- Thin coatings on low-silicon work. On steel below about 0.03% silicon, tubular products and very thin plate in particular, a nickel bath can leave the coating under the specified minimum. The AGA's remedy is to blast-clean that steel so the coating forms on a rougher surface.
- Maintenance. Nickel has to be added regularly and is difficult to hold in the bath, and nickel powder needs special equipment.
- No discrimination. The bath cannot tell one heat from the next. ASTM A123 Note 14 warns that a fabrication mixing steel compositions in the same category and thickness range can make it hard to get the required thickness on its non-reactive steel while avoiding excess on its reactive steel, and tells the galvanizer and purchaser to agree a plan.
The other levers are weaker. Sweep blasting is, in the AGA's words, the surest way to reduce thick coatings on known reactive steel. A shorter immersion or a lower kettle temperature can help, but the AGA is explicit that none of these methods guarantees a thinner coating, and ASTM A385/A385M-20 section 3.5 says the same in its own terms: with the chemistry known beforehand, experienced galvanizers can exercise limited control over these coatings in some instances, not all. In its note on the 2024 A123 revision the AGA adds that a purchaser's request to limit thickness by cutting immersion time is not known to guarantee the result, since immersion time is only one of many variables.
Treat the nickel decision as a one-page proposal, and keep the arithmetic in kilograms per tonne:
- Share of tonnage in the Sandelin region, from your certificates over the last year.
- Zinc saved per tonne on those heats, from the table in the previous section.
- The blended saving, which is share times saving.
- Against it: the dross increase, the rework on low-silicon steel that falls under the minimum, and the nickel itself.
If the blended saving does not clearly beat the list in point 4, the answer is to price the reactive steel, not to change the bath.
Price reactive steel on its own line
A blended rate makes the customers who bring well-behaved steel pay for the ones who do not. The Zinc Consumption KPIs article makes the rule: identify Sandelin steel from the mill certificate and price it separately. The size of the subsidy is easy to state. On 8 mm work a 100 µm coating carries about 22.8 kg of zinc per tonne, so a 50 µm overrun is 50% more zinc on that steel, for the same pickling, the same kettle time and the same rate.
A workable structure has five parts.
- Trigger on the certificate, not the result. ISO 14713-2 category C or D, or a silicon equivalent above NOTE 1's limit, puts the heat on the reactive line. The AGA's wider band of 0.04 to 0.15% is a flag for a test dip. Deciding after the dip turns a price into an argument.
- Quote the driver in zinc. Take the extra zinc per tonne from the table in the previous section for the overrun you expect, then convert it at the day's zinc price. Show the kilograms per tonne on the quotation so the customer sees what is being charged for.
- Base the overrun on your own history. The typical bands are a range of 100 to 200 µm. Your own record of past heats of the same grade and section is better evidence of what this steel will do.
- Agree before dipping. A surcharge added after the coating is on the steel will not survive a dispute.
- Treat a missing certificate as reactive until a test dip or a laboratory analysis says otherwise.
The customer's side of the bargain should be in the same paragraph. Coating above the minimum is accepted. Neither standard sets a maximum. Dull appearance and minor roughness that follow from the steel are not grounds for rejection under A123 section 6.2 or ISO 1461 clause 6.1. Above about 250 µm on thick members, the galvanizer and purchaser should agree a flaking check before dispatch, as described in the coating thickness article.
What to write into the order
Ask for the numbers, agree what happens near the boundaries, and never let a missing certificate default to silence.
- Require the certificate. Heat-numbered mill test reports with silicon and phosphorus reported, before fabrication starts, so a problem heat can be swapped while swapping is cheap. The AGA notes that evaluation from the heat's mill report typically gives the most accurate result.
- Do not write chemistry limits as an acceptance criterion. The AGA's commentary on ASTM A385 says specifiers should not set limits on steel chemistry, because steel in the middle of the Sandelin range or above 0.25% silicon can still give acceptable corrosion protection. ASTM A385/A385M-20 section 3.6 agrees: galvanized coatings are specified for corrosion resistance, not appearance, and the normal and the abnormal coating resist corrosion, for all practical purposes, equally. This is about accepting the coating, not buying the steel: A385 section 3.2 itself recommends silicon targets when steel is bought for galvanizing. Where appearance or thickness genuinely matters, ISO 14713-2 clause 6.2 says to seek specialist advice on steel selection before fabrication.
- State the thickness basis and accept the excess. Name the A123 grade or the ISO 1461 mean, say that coating above the minimum from reactive steel is accepted, and say no maximum applies.
- Plan the mixed fabrication. Where one assembly combines steels of different reactivity, agree the approach in advance, as A123 Note 14 directs.
- Flag thin-coating steel. ASTM A385/A385M-20 section 3.7 names steel with very low silicon, below 0.02%, aluminium-killed steel, and steel with phosphorus below 0.020% as able to fall short of the A123 or A153 minimum, and tells the galvanizer and purchaser to agree a plan: accept the lower thickness, paint over the zinc as a duplex system, blast-clean before galvanizing to thicken the coating, or over-pickle in sulfuric acid to roughen the surface. ASTM A123 eased the burden for plate, and for strip and bar between 6.4 and 16 mm, by setting Grade 75. ISO 1461:2022 clause 6.5 goes further for sections over 3 mm with silicon at or below 0.01% and aluminium above 0.035% that show ultra-low reactivity: the next lower section-thickness row of Table 3 applies, and the declaration of compliance must state the adjusted minimum. The clause's note warns that laser-grade or very smooth steel can give even less.
- Identify the ancillary elements that matter. ISO 1461:2022 Annex A.2 lets the purchaser name any ancillary element, for example a safety-critical bracket, that must be treated as a significant surface and measured.
- Allow a test dip where the chemistry is unknown or doubtful, with the cost agreed in advance.
When the certificate is missing, work down a short list. Look up the grade's chemical requirements table for the range, remembering that a specification range is only general guidance. Ask the fabricator or supplier for the certificate before the steel is dipped. Send a representative sample for independent laboratory analysis. Galvanize a test piece. Until one of those answers comes back, plan and price the lot as reactive.
A model clause to adapt:
The purchaser shall supply heat-numbered mill test reports, reporting silicon and phosphorus, for all steel to be galvanized. Coating thickness shall meet the minimum required by the governing standard and edition named in the order. Thicker coating resulting from steel composition is accepted, no maximum thickness applies, and dull appearance or minor roughness resulting from steel composition is not grounds for rejection. Where a mill test report is not supplied, the galvanizer may treat the lot as reactive for pricing and may require a test dip at the purchaser's cost.
Tools, related reading and sources
The Steel Reactivity Checker reads a certificate against ISO 14713-2 Table 1 and NOTE 1 interactively, and the Coating Thickness Finder gives the minimum the coating has to reach. Both are on the free tools page.
Related reading in this library:
- Coating Thickness: How to Specify, Measure and Verify It
- Duplex Systems: Paint and Powder over Hot-Dip Galvanizing: reactive steel and sweep blasting
- Zinc Consumption KPIs: How to Measure Plant Efficiency
- ASTM A123 and ISO 1461 New Editions: What Changed
- Standards Library and the matte grey coating entry in the Defect Gallery
Standards cited, from the author's licensed copies:
- ASTM A385/A385M-20: sections 3.2 to 3.7 and 4.1. The edition is cited as checked; A385/A385M-22 has since superseded it.
- ISO 14713-2:2020: Table 1 and its notes, clause 6.2
- ASTM A123/A123M-24: section 6.2, Table 1, Note 14
- ISO 1461:2022: clauses 6.1 and 6.5, Annex A.2
Further reading, pages opened on 2026-09-30:
- AGA, Evaluating Steel Chemistry Prior to Galvanizing: silicon equivalent windows
- AGA, Silicon Content of Steel
- AGA, Thinner Galvanized Coatings
- AGA, Alloy Additions to the Kettle and Their Purposes
- AGA, 2024 Revision of ASTM A123: section 6.2, Notes 13 and 14
- AGA, Maximum Coating Thickness
- V&S Galvanizing, Steel Chemistry Evaluation for Hot-Dip Galvanizing: typical thickness by silicon band
- Sperrin Galvanisers, Important Revisions to ISO 1461: clause 6.5 on ultra-low-reactivity steels
The figures apply to batch galvanizing of fabricated articles at normal kettle temperatures. High-temperature galvanizing, continuous lines and fasteners need their own check, and the edition named in the contract governs.
© Aladdin Mohammed · HDG Community. Requirements are quoted from ISO 14713-2:2020, ASTM A385/A385M-20, ASTM A123/A123M-24 and ISO 1461:2022 for batch galvanizing of fabricated articles. The six heats in the certificate table are illustrative. Nothing here replaces the governing standard, the project specification or the edition named in the contract.