Duplex Systems: Paint and Powder over Hot-Dip Galvanizing
Paint or powder over hot-dip galvanizing outlasts both coatings added together, but only when the zinc is prepared for it. Where the 1.5 to 2.3 synergy factor comes from and how the atmosphere sets it, a worked example on the Duplex Life Estimator, sweep blasting and the powder outgassing bake, and the 20 to 30 µm repaint trigger.
Two coatings that protect each other
A duplex system is hot-dip galvanizing with an organic coating over it: liquid paint, powder, or both. It is specified for three reasons: a design life that zinc alone cannot reach in the environment, a colour the client wants, or a colour the site needs for safety or identification. Done properly, it outlasts both of its parts added together. Done badly, the paint loses its grip on the zinc early, and the owner has paid for two coatings to get the protection of one.
This article covers the engineering behind that difference. What it settles:
- ISO 14713-1:2017 clause 6.5 confirms the synergy and explains it in one sentence each way, but publishes no multiplier.
- The multiplier comes from J.F.H. van Eijnsbergen's Duplex Systems (1994): 1.5 to 2.3 times the sum of the two lives, about 1.5 in very aggressive atmospheres and 2.3 in milder ones. A 2011 handbook gives a wider band, 1.2 to 2.5. Neither source ties the factor to an ISO corrosivity category.
- A longer total life does not mean fewer site visits. ISO 14713-1 recommends about 10 years to first maintenance for painted zinc, against 20 years or more for the same zinc left bare, because the paint's appearance goes first.
- The repaint trigger is a measurement, not a date: maintain before any steel rusts and preferably while at least 20 to 30 µm of zinc remains.
- Sweep blasting takes about 10 µm of zinc off the surface, so the coating must be ordered with that loss in mind, and paint should follow within hours, not weeks.
- Powder needs one step that paint does not: an outgassing bake, hotter than the curing oven, before the powder goes on.
Why the synergy works both ways
ISO 14713-1:2017 clause 6.5, "Duplex systems", states the effect directly. The total life of a zinc coating plus an organic coating "is usually significantly greater than the sum of the lives" of the two, and it gives the reason in both directions: the zinc reduces under-rusting of the paint film, and the paint preserves the zinc from early corrosion.
Each coating covers the other's weakness:
- Paint on bare steel fails from its defects. Rust starts at a pore, a scratch or a thin edge and creeps under the film. Iron corrosion products take up far more volume than the steel they came from, so they lift the paint and the failure spreads.
- Zinc on its own fails by being consumed. It corrodes slowly and evenly, at a rate set by the atmosphere, until too little is left to protect the steel.
- Together, the paint slows the zinc's consumption, because the zinc no longer meets the moisture and pollutants directly. Van Eijnsbergen describes the organic coating as protecting the zinc against premature oxidation (p. 7).
- The zinc stops the paint's creep. At a pore or a scratch, zinc corrosion products form instead of rust. The 2011 Handbook of Hot-Dip Galvanization (§10.3, p. 353) notes that they expand far less than iron corrosion products, so they do not lift the coating around a pore or crack, and that they close those pores and cracks as they form.
That is why the combination is not arithmetic. The paint lasts longer because it sits on zinc, and the zinc lasts longer because it sits under paint.
The synergy factor, and what sets it
Van Eijnsbergen gives the relationship as an empirical formula (Duplex Systems, Elsevier 1994, Chapter II, p. 7):
D(duplex) = 1.5 to 2.3 × [ D(zinc) + D(paint) ]
Here D is the durability in years of outdoor exposure until not more than five percent of the underlying steel surface has rusted. D(zinc) and D(paint) are the lives of the zinc coating and of the paint coating each applied directly to steel. On page 8 he sets the factor by atmosphere: about 1.5 in very aggressive atmospheres and 2.3 in less aggressive climates, with relative humidity and the duration of wetness also playing a part. His own example, from Fig. II-1: 70 µm of zinc in an industrial atmosphere lasts about 9 years, 100 µm of paint on bare steel about 3 years, and the duplex system about 18 years. That is the low end, 1.5 times the sum of 12 years.
The second source in this library gives a different band. The Handbook of Hot-Dip Galvanization (Maaß and Peißker, eds., Wiley-VCH 2011, §10.3, p. 353) writes the same relationship as protection periods multiplied by 1.2 to 2.5.
| Source | Factor | What sets the value | End point of "life" |
|---|---|---|---|
| Van Eijnsbergen, Duplex Systems, 1994, pp. 7 to 8 | 1.5 to 2.3 | The atmosphere: about 1.5 very aggressive, 2.3 less aggressive; humidity and wetness also count | Not more than 5% of the steel surface rusted |
| Handbook of Hot-Dip Galvanization, 2011, §10.3, p. 353 | 1.2 to 2.5 | Not stated | "Protection period", not defined further there |
| ISO 14713-1:2017, clause 6.5 | None published | Synergy confirmed in words only | Maintenance before any steel rusting |
Why do the bands differ? The handbook gives the formula without saying which conditions put a system at 1.2 or at 2.5, and without a definition of the end point, so the two bands are not measuring quite the same thing. Van Eijnsbergen's is the narrower band with a stated rule for choosing within it. That is why the site's Duplex Life Estimator uses 1.5 to 2.3.
Two cautions follow:
- Neither source maps the factor to an ISO 9223 category. Van Eijnsbergen's atmospheres are industrial, urban, marine and rural, not C2 to CX. Any table that assigns, say, a single factor to C4 is an interpretation, and no source in this library gives such a figure.
- The factor multiplies years that are themselves estimates. A paint life on bare steel is rarely known to better than a few years, and the zinc life comes from a corrosion-rate band. Treat a duplex life as a planning range.
A worked example on the Duplex Life Estimator
Take a structure in a C5 atmosphere, galvanized to an 85 µm mean coating, with a paint system that would last about 10 years on blasted steel in the same place.
The zinc leg comes from ISO 14713-1:2017 Table 1, which gives zinc corrosion rates of 4.2 to 8.4 µm per year in C5:
Zinc life = 85 ÷ 8.4 to 85 ÷ 4.2 = 10 to 20 years (rounded, as ISO 14713-1 Table 2 does)
Sum of the parts = (10 + 10) to (20 + 10) = 20 to 30 years
Duplex life = 1.5 × 20 to 2.3 × 30 = 30 to 69 years
The Duplex Life Estimator returns exactly that, 30 to 69 years, because it applies 1.5 to the low end and 2.3 to the high end. Now apply Van Eijnsbergen's rule for the atmosphere. C5 is a very aggressive environment, so the factor sits near 1.5 at both ends:
Very aggressive atmosphere: 1.5 × 20 to 1.5 × 30 = 30 to 45 years
That is the number to plan with in C5. The upper part of the tool's range belongs to milder atmospheres. Run the same coating and paint in C4 and the tool returns 45 to 100+ years, with the zinc alone lasting 20 to 40 years. The tool shows the whole band in every category on purpose: the source gives no category mapping, so the choice within the band is the engineer's, and in an aggressive environment the honest choice is the low end.
Two things the example does not say. It does not say when the first repaint falls, which is the next section, and it does not hold if the preparation is wrong. A paint film that loses adhesion in the second year contributes nothing to the sum.
A longer life is not fewer visits
ISO 14713-1:2017 clause 6.5 makes a point that surprises owners. Maintenance usually takes place when a coating loses its appearance, and zinc usually takes longer to degrade than paint. So a zinc coating may be recommended for 20 years or more to first maintenance, while the same coating under paint is recommended for only 10 years, for reasons of the paint's appearance.
A duplex system buys durability, not freedom from maintenance. The first visit is usually a repaint for appearance, made while the zinc underneath is still intact, and that is the cheapest repaint there is: no rust to remove, only a weathered paint film over sound zinc. The same clause adds two practical notes:
- An area of degraded paint can hold moisture and hasten corrosion, particularly on a surface that rain does not wash.
- Where the owner wants a reasonably intact paint layer as the base for maintenance, the original paint system should be applied with extra thickness.
ISO 12944-5 says something similar from the paint side. Its Annex B note on paint systems over hot-dip galvanized steel says that the durability given for such a system relates to the paint's adhesion to the galvanized surface, and that where the paint is damaged, the remaining galvanized layer still protects the steel. A durability class from ISO 12944 is therefore a statement about the paint, not a life for the duplex system.
When to repaint: measure the zinc
ISO 14713-1:2017 clause 6.5 gives the one hard number in this subject. If the life of the zinc coating is to be prolonged, maintenance has to take place before any steel rusting occurs, and preferably while at least 20 to 30 µm of zinc coating remains. If maintenance waits until the zinc is consumed and rust has started, the clause says, the steel has to be maintained in the same way as rusted painted steel, and the duplex advantage is gone.
In practice:
- Inspect the zinc, not the calendar. At each paint inspection, take magnetic gauge readings through the paint on representative areas, or at local breaks after cleaning, and compare them with the as-galvanized readings in the quality records. The paint film itself has to be subtracted from a reading taken over it.
- Watch the edges and the unwashed surfaces. They lose paint first and hold moisture longest.
- Act at the band, not at the first rust. On the 85 µm coating of the example, that means repainting while 20 to 30 µm is still there, so once 55 to 65 µm has gone.
Van Eijnsbergen makes the same point from the maintenance side (p. 9): when only a weathered zinc layer remains and there is no rust, the structure can be reconditioned safely, without relying on doubtful derusting. The cleaning must leave that zinc intact. For weathered duplex structures he recommends low-pressure wet blasting at 1 to 2 bar for large structures such as towers and halls (p. 59), and notes that high-pressure water jets below 100 bar leave the zinc intact while pressures of 400 bar and upwards attack and remove it (p. 60).
Order it as a duplex system
The galvanizer has to know. ASTM A123/A123M-24 sections 6.2 and 6.4 say that the surface roughness of articles to be painted or powder coated, and any smoothing of the coating before coating, shall be mutually determined by the galvanizer and the purchaser. Further preparation, including cleaning, profiling and outgassing, shall follow ASTM D6386 for paint and ASTM D7803 for powder, and is the responsibility of the paint or powder applicator.
The 2011 handbook (§10.5, p. 355) puts the same duty the other way round: the galvanizing shop needs to know the intended duplex design and the intended surface preparation method, because some normal after-treatments spoil adhesion. It names oiling or waxing, and water-bath cooling with white rust formation. ASTM D7803-12 section 5.1.2 says adhesion problems have been experienced on newly galvanized work that was water quenched or chromate treated, and that neither treatment is recommended for work that is to be coated.
What follows for the galvanizer:
- No quench or passivation on duplex work unless the paint system's supplier has approved it.
- Remove what the coating does not need. Drips, runs, dross pimples and high spots become holidays in the paint film. D7803 section 5.1.1 asks for high spots to be smoothed level with the surrounding zinc without removing the base coating, and the thickness then to be checked against A123 or A153.
- Allow for the zinc that preparation removes. The handbook (§10.6.3.1, p. 359) gives a sweep-blast loss of 10 to 15 µm and says the coating should be above the minimum required by ISO 1461 so that it still meets it after sweeping.
- Keep the paint shop close in time. Every hour between the kettle and the paint gun is an hour for zinc oxide, hydroxide and, near the sea or a pickling line, chlorides to form.
Preparing galvanized steel for paint
What has to come off
Fresh zinc reacts with air at once. The handbook (§10.6.1, Table 10.1, p. 357) sorts the products: zinc oxide and zinc carbonate are not critical for adhesion, but zinc hydroxide, chlorides and sulfates are, and all of them look white to light grey, so they cannot be told apart by eye. On the same page it says that weathering the zinc before painting, once common practice, is no longer recommended, because the adhesion-friendly patina cannot be guaranteed or tested.
So preparation has to remove whatever has formed, whether or not it can be seen, together with oil, marker, flux residue, ash and blasting dust.
Sweep blasting
Sweep blasting is a light blast with a fine, non-metallic abrasive that cleans the zinc and roughens it slightly without stripping it. The handbook (§10.6.3.1, p. 359) calls it the safest preparation method and generally applicable. The two sources give close parameters:
| Parameter | Van Eijnsbergen 1994 | Handbook of Hot-Dip Galvanization 2011 |
|---|---|---|
| Air pressure | 1.5 to 2.5 bar (p. 68) | Up to 0.3 MPa, which is 3 bar (p. 359) |
| Nozzle distance | 40 to 50 cm (p. 68) | 0.5 to 0.8 m (p. 359) |
| Angle | A lower angle on alloy-layer coatings (p. 68) | 30° (p. 359) |
| Abrasive | Fine inert grit, 0.2 to 0.5 mm (p. 67) | Non-metallic, 0.2 to 0.5 mm (p. 359) |
| Zinc removed | 8 to 13 µm, average 10 µm (p. 71) | 10 to 15 µm (p. 359) |
| Result | A very homogeneous, rough zinc surface (Fig. V-8, p. 69); the normal procedure removes less than 13% of the coating (p. 71) | Matt grey surface, roughness grade "fine" to ISO 8503-1 (p. 359) |
| Time to first coat | Less than 48 hours after galvanizing in practice, the shorter the better; paint immediately after sweeping (pp. 67, 71) | Immediately after sweeping, at the latest within 24 hours (p. 360) |
Three points from the same pages decide whether the coating survives the blast:
- Reactive steel needs a gentler blast. Van Eijnsbergen lowers the pressure to 1.5 to 1.7 bar and moves the nozzle out to 60 to 70 cm when the coating has the grey look of all-alloy layers, to avoid flaking (p. 68). ASTM D7803-12 section 5.1.3.1 goes further: for reactive steel with all-alloy coatings, even 0.15 to 0.25 MPa can be too much. This is where the mill certificate reaches the paint shop.
- Flaking is a defect, not a side effect. The handbook says zinc flaking during sweeping must be avoided, and any that occurs must be repaired like a galvanizing defect, by thermal zinc spraying or a zinc-dust coating. Repairs made before sweeping get exposed again and need repairing a second time (pp. 359 to 360).
- Thin paint on a swept surface is a risk. Van Eijnsbergen warns that a coating system below 60 to 70 µm dry film can be locally too thin over the swept profile, with poor weather and water resistance as a result (pp. 71 to 72).
Measure before and after. The coating thickness that matters to the owner is the one left under the paint, and the methods are the ones in the coating thickness article.
When the steel has waited
The handbook (§10.6.4.1, pp. 363 to 364) sorts liquid painting by how long the zinc has waited:
- Painted within 24 hours of galvanizing, with no outdoor weathering in between: for one-component paints under normal exposure, local cleaning and dust removal can be enough. Two-component epoxy systems and higher corrosion stress call for sweep blasting.
- After a short intermediate weathering, up to 14 days: high-pressure water or steam cleaning for one-component paints, with local abrasion where white rust has formed; sweep blasting for two-component epoxies and higher stress.
- After longer weathering, for example once erected: the contamination is hard to judge, so assess it first, and sweep blast for two-component systems.
Its conclusion is the useful one for any project: workshop painting straight after galvanizing, or after a short wait, is preferred even when sweep blasting is needed.
Preparing it for powder
Powder adds heat, and heat brings the zinc's trapped gases out. ASTM D7803 is the practice for it. The copy on file is D7803-12; ASTM has since published later editions, so check the contract's edition before quoting the clause numbers below.
Its scope covers new, partially weathered and fully weathered galvanized surfaces on articles galvanized after fabrication, not sheet or coil. Section 4.3 explains the failure it is written to prevent: gases trapped during galvanizing escape through the coating as the powder cures, and unless they are driven out first, the result is pinholes or blisters. Pinholes let chlorides reach the zinc, and the zinc corrosion products can then bleed through as white staining.
The sequence D7803-12 sets out:
- Classify the surface. Newly galvanized means within the previous 48 hours, with no quench or chromate treatment and no visible white oxide or hydroxide (section 5.1). Older work is partially weathered; work exposed for six months or more, with a surface mainly of zinc carbonate, is fully weathered (sections 5.2 and 5.3).
- Smooth and clean. Level high spots and drip lines with hand or power tools, check the thickness, and remove oil and grease (sections 5.1.1 and 5.1.2). Test for a chromate coating if the galvanizer has not said one was avoided (section 5.1.2.1).
- Profile by one of three methods (section 5.1.3): sweep blasting to SSPC-SP 16, whose purpose is "to deform, not remove" the zinc, with the work kept at least 3 °C above the dew point; phosphating; or grinding and sanding with no more than 25 µm removed.
- Coat soon. Fresh zinc oxide forms quickly in humid or hot conditions and cannot be seen, so the powder goes on as soon as possible after preparation.
- Outgas before powdering (section 6.1). Pre-bake the work in an oven that can heat it to 30 °C above the curing-oven temperature, held until the surface reaches it, typically one hour. If the work was phosphated, keep the pre-bake at or below 280 °C, or the phosphate layer breaks down.
- Cool and coat. Cool the work to sufficiently below the curing temperature before the powder is applied.
- Inspect each layer on its own. The galvanized coating must meet A123 or A153 in full, and the zinc and the powder thicknesses are measured independently (section 7.1).
The pre-bake differential is the step plants most often drop, because it costs oven time. It is also the step that decides whether a powder coat over galvanizing has pinholes.
What to put in the order
For the purchaser and the specifier, a duplex order needs the following, in writing:
- The system as a whole. Galvanizing standard and edition, paint or powder system, and who prepares the surface.
- Duplex flagged to the galvanizer. No quench or chromate passivation, smoothing to the agreed finish, and handling that avoids wet storage.
- The coating thickness after preparation. The standard minimum still applies after sweep blasting, so order enough zinc to lose 10 to 15 µm.
- The preparation method and the time limits. For paint, sweep blasting or the method the paint supplier approves, with the paint applied within the agreed number of hours. For powder, the D7803 sequence including the outgassing pre-bake.
- The maintenance trigger. Inspect the zinc and repaint while 20 to 30 µm remains, as ISO 14713-1 clause 6.5 recommends.
- The life estimate as a range, with the factor chosen for the atmosphere: near 1.5 in an aggressive environment.
Related reading in this library:
- Duplex Life Estimator and Galvanizing Lifetime Estimator
- Coating Thickness: How to Specify, Measure and Verify It
- Silicon, Sandelin and Sebisty: Reading the Mill Certificate Before It Costs You
- Corrosion Protection for Steel: Every Method Compared to Hot-Dip Galvanizing
Sources, from the author's own copies:
- ISO 14713-1:2017 (BS EN ISO 14713-1:2017): clause 6.5 and Table 1
- ASTM A123/A123M-24: sections 6.2 and 6.4
- ASTM D7803-12: sections 4.3, 5.1 to 5.3, 6.1 and 7.1. Later editions exist and were not checked here.
- ISO 12944-5:2018 (BS EN ISO 12944-5:2018): Annex B, note on paint systems over hot-dip galvanized steel
- J.F.H. van Eijnsbergen, Duplex Systems: Hot-dip Galvanizing plus Painting, Elsevier, 1994: pp. 7 to 9 and Chapter V, pp. 57 to 72
- P. Maaß and P. Peißker (eds.), Handbook of Hot-Dip Galvanization, Wiley-VCH, 2011: Chapter 10, §10.3 and §10.5 to §10.6, pp. 353 to 364
The figures apply to batch galvanizing of fabricated articles. The paint or powder supplier's data sheet governs its own product, and the edition named in the contract governs the standards.
© Aladdin Mohammed · HDG Community. Figures are quoted from ISO 14713-1:2017, ASTM A123/A123M-24, ASTM D7803-12, ISO 12944-5:2018, J.F.H. van Eijnsbergen's Duplex Systems (1994) and the Handbook of Hot-Dip Galvanization (2011), for batch galvanizing of fabricated articles. Duplex lives are planning estimates, not warranties. Nothing here replaces the governing standard, the coating supplier's data sheet or the edition named in the contract.